Rare earth magnets made from neodymium iron boron (NdFeB) corrode fast because of their own microstructure. A reactive, neodymium-rich phase sits between the magnetic grains and oxidizes first. Air alone starts the attack, and moisture speeds it up. Once those grain boundaries break down, the grains loosen and the magnet fails from the inside. A plated barrier of nickel, copper and nickel (Ni-Cu-Ni) seals the porous surface and keeps air and moisture away from that phase. For some applications, like medical devices, additional metals such as gold can be added as the final layer.
Quick answer
NdFeB rare earth magnets corrode because the neodymium-rich phase at their grain boundaries oxidizes on contact with air, and moisture turns it into a galvanic cell with the iron-rich grains. Ni-Cu-Ni plating seals the porous magnet surface under a continuous metal barrier. For medical devices, a gold layer can go over the Ni-Cu-Ni stack to give the magnet a biocompatible, inert exterior.
Why rare earth magnets corrode so fast
Sintered NdFeB is not one uniform material. It is a mix of phases with very different electrochemical behavior, and that difference drives the corrosion.
What happens inside an NdFeB magnet
Most of the magnet is iron-rich Nd2Fe14B grains. Around 5% is a neodymium-rich phase that sits at the grain boundaries, according to a corrosion study from the Danish Technological Institute. Neodymium’s electrode potential is close to magnesium’s, roughly 1.8 V away from iron.
Exposure to air is enough to oxidize that boundary phase. Add moisture and the two phases form an internal galvanic cell, which speeds the attack. The grains lose their bond, and the magnet can shed powder and lose both strength and magnetic output.
Does a magnetized magnet corrode faster?
It can. In the same study, magnetized samples lost more weight in 3.5% NaCl than non-magnetized ones. The researchers suggest the field helps move oxygen to the surface. Their conclusion for designers is direct: NdFeB needs a barrier-type surface treatment or full encapsulation.
How fast does an uncoated magnet corrode?
Very fast. In accelerated corrosion testing, an unprotected NdFeB magnet shows signs of corrosion almost immediately.
Why bare magnets have to arrive corrosion-free
Corrosion that starts before plating makes the magnet difficult to plate and will most likely cause the process to fail. For that reason, ProPlate® sets strict packaging requirements for bare magnets, whether we order them or customers send them in. Magnets should arrive vacuum sealed and packed so the parts cannot knock against each other.
How Ni-Cu-Ni plating protects NdFeB magnets
The main job of the Ni-Cu-Ni stack is to seal the porosity of the sintered magnet. Ni-Cu-Ni is the industry standard for NdFeB, and our process builds on that standard stack with a few refinements of its own. Each layer has a specific role.
What each layer does
- First nickel layer. Bonds to the prepared magnet surface and forms the base for the rest of the stack.
- Copper layer. Seals porosity. Copper is soft and ductile, so it builds up evenly over the rough sintered surface and closes the paths that moisture and air would otherwise follow to the magnet.
- Outer nickel layer. Protects the copper underneath. Copper oxidizes and corrodes easily, and copper does not diffuse through nickel, so the outer nickel keeps the copper sealed in. It also gives the part a hard, corrosion-resistant surface in service.
Why plating instead of parylene or a titanium enclosure?
Parylene is a common sealing method, but NdFeB porosity can leave pinholes in it. Every pinhole is a path for moisture to reach the neodymium-rich phase. A titanium enclosure is another option: a sealed casing that surrounds the magnet. Electroplating seals the magnet surface itself, with no separate housing around the part.
Why NdFeB is hard to plate
The surface oxide on NdFeB has to come off before any plating will adhere, and removing it takes both acidic and basic chemistries. The catch is that the same chemistry can attack the magnet. ProPlate® developed a pretreatment for NdFeB magnet plating that is aggressive enough for strong adhesion and mild enough to avoid corroding the base material. Porosity is the second problem, handled with plating method selection, agitation and custom fixtures.
Where gold fits
NdFeB on its own is not biocompatible. A magnet that goes into the body needs a biocompatible exterior over a hermetically sealed stack. That is where gold comes in.
Gold is inert, so it does not corrode in the body, and it is a well-established metal in medical device coatings. On a medical magnet, the gold layer goes over the Ni-Cu-Ni stack and adds a biocompatible layer to it. For most industrial magnets, Ni-Cu-Ni alone is the finish. Some applications add a thin rhodium layer instead, for its hardness.
How plated magnets are inspected
Plated magnets go through cross-section inspection, adhesion testing to ASTM B571 and accelerated corrosion porosity testing. Each check looks at the same question from a different angle: is the stack bonded, continuous and free of pores?
A completely sealed magnet should last the life of the part. Constant friction or wear on the plated surface can shorten that, so service life depends on the application.
Where plated NdFeB magnets are used
Plated NdFeB shows up across medical and industrial products:
- Medical devices: catheter navigation, where magnets in the catheter tip are steered by external magnetic systems, plus tumor localization, open MRI, short- and long-term implants and endoscopic assemblies.
- Motors and generators. High-energy NdFeB magnets let designers shrink motor size and weight, and plating protects them in humid or washdown environments.
- Sensors. Hall-effect position and speed sensors in automotive systems, flow meters and industrial encoders, where the magnet faces oil, coolant or humid air for years.
- Hard drives and other electronics, where a sealed, stable surface matters over the life of the product.
Demand for domestic plating of these magnets is growing as buyers look for stateside supply.
FAQs
What are rare earth magnets made of?
Most rare earth magnets are neodymium iron boron (NdFeB). Samarium cobalt (SmCo) is the other main type, and we plate both. NdFeB is the stronger and more widely used of the two, and also the one more prone to corrosion.
Do neodymium magnets rust?
Yes. NdFeB is mostly iron, and its neodymium-rich grain boundaries oxidize even in dry air. Humidity speeds the damage, which spreads along the grain boundaries until the surface starts to crumble.
What is the best coating for neodymium magnets?
It depends on where the magnet will be used. Electroplated nickel and zinc are the most common coatings for sintered NdFeB, and epoxy is also used. Ni-Cu-Ni is the industry standard barrier because it seals porosity. For implants and other parts that contact the body, a gold layer over Ni-Cu-Ni adds a biocompatible, inert exterior.
Can gold be plated directly onto an NdFeB magnet?
No. Gold is porous, so the base material would diffuse through it. The Ni-Cu-Ni stack hermetically seals the magnet first, and gold goes on top of that seal.
How long does Ni-Cu-Ni plating protect an NdFeB magnet?
If the magnet is completely sealed, the plating should protect it for the life of the part. Constant friction can wear through the plating and shorten that, so the answer depends on how the magnet is used.
Is plated NdFeB safe for medical implants?
Bare NdFeB is not biocompatible. With a hermetic, biocompatible exterior such as gold over Ni-Cu-Ni, plated magnets are used in implants and catheter navigation. Biocompatibility of the finished device still has to be confirmed by the device maker. ProPlate® holds ISO 13485:2016 certification.
Talk to us about your magnets
Have an NdFeB part that needs a corrosion barrier, or a medical magnet that needs a biocompatible finish? Send your drawing through Request a Quote and our team will review your magnet and application.